来自英国七个脊柱中心的取出式磁控生长棒分析
研究对来自英国七个脊柱中心的18名儿童取出的34根MAGEC生长棒进行独立分析,以明确早期起病脊柱侧凸治疗中的失效模式。所有34根棒内部均发现钛磨损碎屑(100%),91%出现延伸杆可测量磨损,74%径向轴承严重损坏,53% O型圈密封失效,44%驱动销断裂但被认为是失效结果而非原因。结论提出高量钛磨损碎屑合并O型圈密封损坏可能解释临床报道的金属沉着症,并提出基于脊柱自然离轴载荷的失效机制。
要点
- 全部34根(100%)取出MAGEC棒内部均发现钛磨损碎屑,31/34(91%)延伸杆朝向磁体端有可测量磨损。
- 25/34(74%)MAGEC棒内部径向轴承严重损坏,18/34(53%)出现O型圈密封失效,15/34(44%)驱动销断裂(被认为是失效结果而非原因)。
- 高量钛磨损碎屑合并O型圈密封损坏可能解释临床报道的MAGEC棒周围金属沉着症。
核心结论
- 高量钛磨损碎屑合并O型圈密封损坏可能解释临床报道的部分MAGEC棒周围金属沉着症。
- 基于取出物数据,提出MAGEC棒因脊柱自然离轴载荷而发生失效的机制。
- 这是迄今报道的取出MAGEC棒完整分析的最大数据集。
研究设计与样本
- 对取出的MAGEC生长棒进行独立分析。
- 从英国七个脊柱中心获取34根MAGEC棒,来自18名儿童,取出原因包括棒延长失败和达到最大棒撑开。
- 切开棒以评估内部组件。
主要发现
- 外部所有MAGEC棒在延伸杆组件上均显示局部标记,称为「生长标记」,提示棒在体内生长。
- 切开后,全部34根(100%)MAGEC棒内部均发现钛磨损碎屑。
- 31/34(91%)MAGEC棒显示延伸杆朝向磁体端的可测量磨损。
- 25/34(74%)MAGEC棒内部可见径向轴承严重损坏,18/34(53%)出现O型圈密封失效。
- 15/34(44%)MAGEC棒驱动销断裂,但被认为是棒失效的结果而非原因。
局限性
- 证据等级为4。
以上解读依据论文摘要(全文未开放获取或许可不允许翻译转载)。
原文
STUDY DESIGN: Analysis of explanted MAGnetic Expansion Control (MAGEC) growing rods. OBJECTIVE: To analyze explanted MAGEC rods used in management of early onset scoliosis and identify the mode of failure in such cases. SUMMARY OF BACKGROUND DATA: Magnetically controlled growing rods are increasingly used as the option of choice for early onset scoliosis. However, being more complex than conventional growing rods they are perhaps more likely to succumb to multifarious failure modes. In addition, metallosis has been reported around failed MAGEC rods. METHODS: Explanted MAGEC rods from seven UK spinal centers were obtained for independent analysis. Thirty-four MAGEC rods, from 18 children, explanted for reasons including failure of rod lengthening and maximum rod distraction reached, were cut open to allow internal components to be evaluated and assessed. RESULTS: Externally, all MAGEC rods showed localized marks, which were termed "growth marks" as they indicated growth of the rod in vivo, on the extending bar component. After cutting open, titanium wear debris was found inside all 34 (100%) MAGEC rods. Ninety-one percent (31/34) of MAGEC rods showed measurable wear of the extending bar, towards the magnet end. Substantial damage to the radial bearing was seen inside 74% (25/34) of MAGEC rods while O-ring seal failure was seen in 53% (18/34) of cases. In 44% (15/34) of MAGEC rods the drive pin was fractured but this was felt to be an effect of rod failure, not a cause. CONCLUSION: The combination of high volumes of titanium wear debris alongside O-ring seal damage likely accounts for the metallosis reported clinically around some MAGEC rods. Based on this explant data, a failure mechanism in MAGEC rods due to the natural off axis loading in the spine was proposed. This is the largest data set reporting a complete analysis of explanted MAGEC rods to date. LEVEL OF EVIDENCE: 4.
引用
- Joyce TJ, Smith SL, Rushton PRP, et al. Analysis of Explanted Magnetically Controlled Growing Rods From Seven UK Spinal Centers. Spine (Phila Pa 1976). 2018. PMID: 28459777. doi:10.1097/BRS.0000000000002221
供执业医师工作参考,不替代临床判断;数值与分级以指南原文为准。