植入超过10年的高交联聚乙烯髋臼内衬的股骨头穿透率与氧化
研究分析了49例因翻修取出的第一代高交联聚乙烯髋臼内衬,比较退火与重熔两种工艺的穿透率和氧化指数。退火组平均植入13.1±2.6年,重熔组12.1±1.7年;穿透率分别为0.0177±0.014 mm/年和0.015±0.022 mm/年,两组无显著差异(P=0.28)。退火组各区域氧化指数均显著高于重熔组(P<0.001),但氧化较高似乎未导致更大磨损。
要点
- 退火与重熔高交联聚乙烯内衬的股骨头穿透率相似(P=0.28),平均穿透率均较低。
- 退火组在边缘、锁定机制、关节面和背侧区域的氧化指数均显著高于重熔组(P<0.001)。
- 氧化程度较高似乎未伴随更大的磨损。
核心结论
- 退火高交联聚乙烯的氧化程度高于重熔高交联聚乙烯,但氧化较高似乎未导致更大磨损,两组平均穿透率均较低且相似。
研究设计与样本
- 经机构审查委员会批准的植入物取出项目,共取回49例全髋关节置换髋臼内衬。
- 穿透率计算为未负载区与负载区厚度之差除以植入时间。
- 采用傅里叶变换红外光谱按美国材料与试验协会2102标准测量边缘、锁定机制、关节面和背侧区域的氧化指数。
- 使用Mann-Whitney U检验比较退火与重熔组件的统计学差异。
主要发现
- 退火组件平均植入时间为13.1±2.6年,重熔组件为12.1±1.7年。
- 翻修最常见原因为聚乙烯磨损、不稳定和松动。
- 退火组件平均穿透率为0.0177±0.014 mm/年,重熔组件为0.015±0.022 mm/年。
- 重熔与退火队列的穿透率无差异(P=0.28)。
- 退火队列所有感兴趣区域的氧化指数均显著更高(P<0.001)。
局限性
- 原文未报告局限性。
以上解读依据论文摘要(全文未开放获取或许可不允许翻译转载)。
原文
BACKGROUND: Highly cross-linked polyethylene (HXLPE) was introduced to improve wear in total hip arthroplasty, with manufacturers implementing different thermal treatments to reduce oxidation. It is important to understand how long-term time in vivo affects the wear of these materials. The purpose of this study was to investigate the wear and oxidative performance of first-generation HXLPE hip inserts implanted for greater than 10 years and compare annealed and remelted HXLPE formulations. METHODS: There were 49 total hip arthroplasty liners retrieved during routine revision surgery as part of an institutional review board-approved implant retrieval program. Penetration rates for the liners were calculated as the difference between the thickness of the unloaded and loaded regions divided by implantation time. Oxidation indices for the rim, locking mechanism, articulating surface, and backside regions were measured using Fourier-transform infrared spectroscopy according to American Society for Testing and Materials 2102. Mann-Whitney U tests were used to determine the statistical difference between annealed and remelted components. RESULTS: The cohort had an average implantation time of 13.1 ± 2.6 years for annealed and 12.1 ± 1.7 years for remelted components. The components were revised most often for polyethylene wear, instability, and loosening. The penetration rate averaged 0.0177 ± 0.014 mm/year for annealed components and 0.015 ± 0.022 mm/year for remelted components. Penetration rates did not differ between the remelted and annealed cohorts (P = .28). Oxidation indices were found to be significantly higher in the annealed cohort for all regions of interest (P < .001). CONCLUSIONS: Oxidation was found to be higher in the annealed HXLPE; however, this does not seem to be associated with greater wear as we found the average penetration rates for the cohorts were low, and the penetration rates were similar between the annealed and remelted cohorts.
引用
- Derr T, MacDonald DW, Malkani AL, et al. Femoral Head Penetration Rates and Oxidation of Highly Cross-Linked Polyethylene Hip Liners Implanted More Than 10 Years. J Arthroplasty. 2024. PMID: 38754708. doi:10.1016/j.arth.2024.05.024
供执业医师工作参考,不替代临床判断;数值与分级以指南原文为准。