文献速递关节外科

模块化双动髋臼内衬的微动与摩擦腐蚀:设计、微观结构和就位不良的作用

Fretting and Tribocorrosion of Modular Dual Mobility Liners: Role of Design, Microstructure, and Malseating.
PubMed 文献 · J Arthroplasty · 2024-04-17

本研究对28例平均体内留存14.6个月的模块化双动髋臼植入物进行回收分析,发现25%的内衬存在影像学就位不良且均属同一设计(P = .01),就位不良是增加体积材料丢失的独立危险因素(P = .017),特定设计特征可能使内衬更易就位不良。

要点

  • 28例回收模块化双动植入物中,7例(25%)内衬存在影像学就位不良,且均为同一设计(P = .01)。
  • 就位不良是锥度处体积材料丢失增加的独立危险因素(P = .017)。
  • 6例(22%)为重度4级腐蚀,6例(22%)为中度3级,11例(41%)为轻度2级,5例(18.5%)为1级或无可见腐蚀。

核心结论

  • 双动髋臼摩擦腐蚀伴可量化材料丢失在就位不良的内衬中更常见。
  • 特定设计特征可能使内衬更易发生就位不良。
  • 就位机制、内衬特征与患者因素之间的相互作用可能促成外壳/内衬摩擦腐蚀环境。

研究设计与样本

  • 评估28例回收的模块化双动植入物,平均体内留存时间14.6个月(范围1至83个月)。
  • 纳入2家制造商(分别为12例和16例内衬)。
  • 术后X线片上内衬与外壳之间出现明显分离即判定为就位不良。
  • 采用改良Goldberg评分进行定性分析,并使用光学坐标测量机进行定量分析。
  • 每家制造商取一个髋臼外壳进行金相分析。

主要发现

  • 6例植入物(22%)为重度4级腐蚀,6例(22%)为中度3级,11例(41%)为轻度2级,5例(18.5%)为1级或无可见腐蚀。
  • 锥度处平均体积材料丢失为0.086 ± 0.19 mm3。
  • 7例内衬(25%)有影像学就位不良证据,且均为同一设计(P = .01)。
  • 两种内衬设计在钴铬合金类型、锥度表面光洁度和形状偏差方面存在根本差异。
  • 就位不良是体积材料丢失增加的独立危险因素(P = .017)。

局限性

  • 证据等级为III级。

以上解读依据论文摘要(全文未开放获取或许可不允许翻译转载)。

原文

BACKGROUND: Modular dual mobility (DM) bearings have a junction between a cobalt chrome alloy (CoCrMo) liner and titanium shell, and the risk of tribocorrosion at this interface remains a concern. The purpose of this study was to determine whether liner malseating and liner designs are associated with taper tribocorrosion. METHODS: We evaluated 28 retrieved modular DM implants with a mean in situ duration of 14.6 months (range, 1 to 83). There were 2 manufacturers included (12 and 16 liners, respectively). Liners were considered malseated if a distinct divergence between the liner and shell was present on postoperative radiographs. Tribocorrosion was analyzed qualitatively with the modified Goldberg Score and quantitatively with an optical coordinate-measuring machine. An acetabular shell per manufacturer was sectioned for metallographic analysis. RESULTS: There were 6 implants (22%) that had severe grade 4 corrosion, 6 (22%) had moderate grade 3, 11 (41%) had mild grade 2, and 5 (18.5%) had grade 1 or no visible corrosion. The average volumetric material loss at the taper was 0.086 ± 0.19 mm3. There were 7 liners (25%) that had radiographic evidence of malseating, and all were of a single design (P = .01). The 2 liner designs were fundamentally different from one another with respect to the cobalt chrome alloy type, taper surface finish, and shape deviations. Malseating was an independent risk factor for increased volumetric material loss (P = .017). CONCLUSIONS: DM tribocorrosion with quantifiable material loss occurred more commonly in malseated liners. Specific design characteristics may make liners more prone to malseating, and the interplay between seating mechanics, liner characteristics, and patient factors likely contributes to the shell/liner tribocorrosion environment. LEVEL OF EVIDENCE: Level III.

来源:J Arthroplasty,查看原文。版权归原作者所有。

引用

  1. Terhune EB, Serino J, Hall DJ, et al. Fretting and Tribocorrosion of Modular Dual Mobility Liners: Role of Design, Microstructure, and Malseating. J Arthroplasty. 2024. PMID: 38640966. doi:10.1016/j.arth.2024.04.045

供执业医师工作参考,不替代临床判断;数值与分级以指南原文为准。