聚乙烯双动髋臼内衬早期翻修取出物显示聚乙烯变化极小
该研究对37例植入超过2年的双动髋臼内衬进行取回分析,测量内、外承重面的交联密度与氧化指数。结果显示内、外承重面交联密度中位数相似(0.17 mol/dm³ vs 0.17 mol/dm³,P=.6),内承重面氧化指数高于外承重面(0.16 vs 0.13,P=.008),氧化指数与交联密度呈负相关(r=-0.50,P=.002)。作者认为平均3年失败时氧化水平低,不太可能影响材料力学性能。
要点
- 37例双动髋臼内衬取回物平均植入35个月(范围24-96个月)。
- 内、外承重面交联密度中位数相似(0.17 mol/dm³ vs 0.17 mol/dm³,P=.6)。
- 内承重面氧化指数高于外承重面(0.16 vs 0.13,P=.008),氧化指数与交联密度负相关(r=-0.50,P=.002)。
核心结论
- 双动髋臼内衬内、外承重面之间氧化存在小差异,平均3年失败时氧化水平低,不太可能影响材料力学性能。
研究设计与样本
- 收集37例植入时间大于2年的双动髋臼内衬取回物,从病历回顾收集临床与人口学数据,在衬垫顶点取圆柱体并切成长4.5 mm的内、外径段进行交联密度溶胀比测试,用傅里叶变换红外光谱测量100 μm矢状面切片氧化指数,采用Student t检验比较承重面间氧化指数与交联密度差异,用Spearman相关评估患者人口学数据与氧化指数、交联密度的关系。
- 队列平均植入时间为35个月(范围24-96个月)。
主要发现
- 内、外承重面交联密度中位数相似(0.17 mol/dm³ vs 0.17 mol/dm³,P=.6)。
- 内承重面氧化指数高于外承重面(0.16 vs 0.13,P=.008)。
- 氧化指数与交联密度呈负相关(r=-0.50,P=.002)。
局限性
- 原文未报告局限性。
以上解读依据论文摘要(全文未开放获取或许可不允许翻译转载)。
原文
BACKGROUND: Dual mobility (DM) liners were introduced to reduce instability in total hip arthroplasty. They were found to allow for motion predominantly at the femoral head and the inner bearing of the acetabular liner; however, little is known if this motion is sufficient to alter polyethylene material characteristics. We assessed cross-link (XL) density and oxidation index (OI) measurements of the inner and outer bearing articulations. METHODS: Thirty-seven DM liners were collected with a duration of implantation greater than 2 years. Clinical and demographic data were collected from a chart review. A cylinder was cored from the apex of each liner and cut into 4.5 mm long inner and outer diameter segments for XL density swell ratio testing. The OI was measured from sagittal 100 μm microtome slices using Fourier transform infrared spectroscopy. Student's t-tests were used to determine differences in OI and XL density between the bearings. Spearman's correlation assessed relationships between patient demographics, OI, and XL density. Duration of implantation for the cohort was a mean of 35 (range, 24-96) months. RESULTS: The inner and outer bearing had similar median XL densities (0.17 mol/dm3 versus 0.17 mol/dm3, P = .6). The inner bearing had an increased OI when compared to the outer bearing (0.16 versus 0.13, P = .008). The OI was inversely correlated with XL density (r = -0.50, P = .002). CONCLUSION: Small differences were found in oxidation between the inner and outer bearing of the DM construct. Failures at an average of 3 years indicate low levels of oxidation, unlikely to impact the mechanical properties of the material.
引用
- Zlotnicki JP, Baral EC, Westrich GH, et al. Polyethylene Dual Mobility Liners Show Minimal Polyethylene Changes in Early Retrievals. J Arthroplasty. 2023. PMID: 36878437. doi:10.1016/j.arth.2023.02.068
供执业医师工作参考,不替代临床判断;数值与分级以指南原文为准。