一种新型纳米结构钛植入物表面在羊模型中增强骨整合
该研究在8只成年羊的股骨和胫骨中植入碱性热处理(AHT)或羟基磷灰石涂层多孔钛(PCHA)植入物,12周后通过生物力学、微CT和组织形态计量学评估骨整合。结果提示AHT植入物在松质骨和皮质骨的界面剪切强度均高于PCHA植入物,但部分微CT参数无差异。作者认为AHT表面在羊模型中骨整合更强,可为后续临床非劣效性研究提供伦理基线。
要点
- 松质骨界面剪切强度AHT组9.3 MPa vs PCHA组7.7 MPa,AHT高1.6 MPa(95%CI 0.5至2.8;p=0.006)。
- 皮质骨界面剪切强度AHT组25.5 MPa vs PCHA组18.9 MPa,AHT高6.6 MPa(95%CI 5.0至8.1;p<0.001)。
- 皮质骨内侧骨-植入物接触百分比AHT组58.1% vs PCHA组46.2%,AHT高11.8%(95%CI 7.1%至16.6%;p<0.001)。
核心结论
- 在羊模型中植入12周后,AHT表面的骨整合强于PCHA表面。
研究设计与样本
- 在8只骨骼成熟羊的股骨和胫骨骨干骺端松质骨(每种植入物16枚;干涉配合)及胫骨骨干三个骨干位置(每种植入物24枚;线对线配合)手术植入AHT和PCHA植入物。
- 术后12周取出骨骼,通过生物力学推穿测试、微CT和组织形态计量学评估AHT与PCHA植入物的骨整合。
- 采用线性混合效应模型分别对皮质骨和松质骨组进行比较,模型包含动物随机效应、术前体重协变量及植入位置协变量,显著性水平设为α=0.05。
主要发现
- 松质骨界面剪切强度估计边际均值AHT组9.3 MPa vs PCHA组7.7 MPa,AHT高1.6 MPa(95%CI 0.5至2.8;p=0.006)。
- 皮质骨界面剪切强度估计边际均值AHT组25.5 MPa vs PCHA组18.9 MPa,AHT高6.6 MPa(95%CI 5.0至8.1;p<0.001)。
- 松质骨骨-植入物接触百分比AHT组55.1% vs PCHA组58.7%,调整后估计边际均值差-3.6%(95%CI -8.1%至0.9%;p=0.11),未检测到差异。
- 皮质骨内侧骨-植入物接触百分比估计边际均值AHT组58.1% vs PCHA组46.2%,AHT高11.8%(95%CI 7.1%至16.6%;p<0.001);外侧AHT组75.8% vs PCHA组74.9%,调整后估计边际均值差0.9%(95%CI -3.8%至5.7%;p=0.70),无差异。
关键数值与推荐
- 主要结局为界面剪切强度和骨-植入物接触百分比(按微CT方案定义);次要结局为刚度、峰值载荷、失效能量及微CT参数(骨体积/总体积、骨小梁厚度、骨小梁数量)和组织形态计量学参数(骨-植入物接触)。
临床怎么用
- 作者认为,鉴于AHT植入物在皮质骨和松质骨中形成的界面比PCHA植入物更牢固,现可开展使用相同几何形状股骨柄的临床非劣效性研究来比较本研究所用表面。
- 作者认为,鉴于碱性热处理表面具有减少假体周围关节感染和增强植入物骨整合的潜力,本临床前研究结果为开展此类临床研究提供了伦理基线。
局限性
- 原文未报告局限性。
以上解读依据论文摘要(全文未开放获取或许可不允许翻译转载)。
原文
BACKGROUND: A nanostructured titanium surface that promotes antimicrobial activity and osseointegration would provide the opportunity to create medical implants that can prevent orthopaedic infection and improve bone integration. Although nanostructured surfaces can exhibit antimicrobial activity, it is not known whether these surfaces are safe and conducive to osseointegration. QUESTIONS/PURPOSES: Using a sheep animal model, we sought to determine whether the bony integration of medical-grade, titanium, porous-coated implants with a unique nanostructured surface modification (alkaline heat treatment [AHT]) previously shown to kill bacteria was better than that for a clinically accepted control surface of porous-coated titanium covered with hydroxyapatite (PCHA) after 12 weeks in vivo. The null hypothesis was that there would be no difference between implants with respect to the primary outcomes: interfacial shear strength and percent intersection surface (the percentage of implant surface with bone contact, as defined by a micro-CT protocol), and the secondary outcomes: stiffness, peak load, energy to failure, and micro-CT (bone volume/total volume [BV/TV], trabecular thickness [Tb.Th], and trabecular number [Tb.N]) and histomorphometric (bone-implant contact [BIC]) parameters. METHODS: Implants of each material (alkaline heat-treated and hydroxyapatite-coated titanium) were surgically inserted into femoral and tibial metaphyseal cancellous bone (16 per implant type; interference fit) and in tibial cortices at three diaphyseal locations (24 per implant type; line-to-line fit) in eight skeletally mature sheep. At 12 weeks postoperatively, bones were excised to assess osseointegration of AHT and PCHA implants via biomechanical push-through tests, micro-CT, and histomorphometry. Bone composition and remodeling patterns in adult sheep are similar to that of humans, and this model enables comparison of implants with ex vivo outcomes that are not permissible with humans. Comparisons of primary and secondary outcomes were undertaken with linear mixed-effects models that were developed for the cortical and cancellous groups separately and that included a random effect of animals, covariates to adjust for preoperative bodyweight, and implant location (left/right limb, femoral/tibial cancellous, cortical diaphyseal region, and medial/lateral cortex) as appropriate. Significance was set at an alpha of 0.05. RESULTS: The estimated marginal mean interfacial shear strength for cancellous bone, adjusted for covariates, was 1.6 MPa greater for AHT implants (9.3 MPa) than for PCHA implants (7.7 MPa) (95% CI 0.5 to 2.8; p = 0.006). Similarly, the estimated marginal mean interfacial shear strength for cortical bone, adjusted for covariates, was 6.6 MPa greater for AHT implants (25.5 MPa) than for PCHA implants (18.9 MPa) (95% CI 5.0 to 8.1; p < 0.001). No difference in the implant-bone percent intersection surface was detected for cancellous sites (cancellous AHT 55.1% and PCHA 58.7%; adjusted difference of estimated marginal mean -3.6% [95% CI -8.1% to 0.9%]; p = 0.11). In cortical bone, the estimated marginal mean percent intersection surface at the medial site, adjusted for covariates, was 11.8% higher for AHT implants (58.1%) than for PCHA (46.2% [95% CI 7.1% to 16.6%]; p < 0.001) and was not different at the lateral site (AHT 75.8% and PCHA 74.9%; adjusted difference of estimated marginal mean 0.9% [95% CI -3.8% to 5.7%]; p = 0.70). CONCLUSION: These data suggest there is stronger integration of bone on the AHT surface than on the PCHA surface at 12 weeks postimplantation in this sheep model. CLINICAL RELEVANCE: Given that the AHT implants formed a more robust interface with cortical and cancellous bone than the PCHA implants, a clinical noninferiority study using hip stems with identical geometries can now be performed to compare the same surfaces used in this study. The results of this preclinical study provide an ethical baseline to proceed with such a clinical study given the potential of the alkaline heat-treated surface to reduce periprosthetic joint infection and enhance implant osseointegration.
引用
- Jones CF, Quarrington RD, Tsangari H, et al. A Novel Nanostructured Surface on Titanium Implants Increases Osseointegration in a Sheep Model. Clin Orthop Relat Res. 2022. PMID: 36001022. doi:10.1097/CORR.0000000000002327
供执业医师工作参考,不替代临床判断;数值与分级以指南原文为准。