次氯酸钠与EDTA序贯暴露对人牙本质磷灰石和胶原降解深度的定量FTIR研究
该研究用ATR-FTIR光谱定量分析人牙本质颗粒经2.5%NaOCl和17%EDTA暴露后胶原与磷酸盐的降解深度。结果显示NaOCl快速消耗表面胶原,EDTA导致磷酸盐丢失,两者序贯使用可加深侵蚀深度。
要点
- NaOCl暴露2分钟即致表面胶原下降约40%,6-10分钟平台期约60%。
- 10分钟NaOCl处理平均胶原丢失深度为16±13 μm。
- 10分钟EDTA致表面磷酸盐丢失约60%,平均深度19±12 μm;1440分钟达89±43 μm。
核心结论
- NaOCl消耗胶原、EDTA消耗磷灰石,序贯暴露可同时暴露另一组分并加深侵蚀深度。
研究设计与样本
- 每个粒径取250 mg与5 mL 2.5% NaOCl反应2-10分钟,或与17% EDTA反应5-1440分钟。
- 大于75 μm的粉末还接受NaOCl/EDTA/NaOCl各10分钟的序贯暴露。
- 所有实验重复五次,反应后洗涤干燥,大于75 μm颗粒再研磨。
主要发现
- NaOCl暴露2分钟内表面胶原分数下降约40%,6-10分钟平台期约60%。
- 10分钟NaOCl处理平均胶原丢失深度为16±13 μm。
- 10分钟EDTA致表面磷酸盐丢失约60%,平均深度19±12 μm;1440分钟EDTA平均深度89±43 μm。
- 序贯NaOCl/EDTA产生62±28 μm厚的磷酸盐耗竭表面。
- 序贯NaOCl/EDTA/NaOCl导致约85 μm的胶原丢失。
临床怎么用
- 临床使用NaOCl和EDTA冲洗时需注意二者序贯应用可能加深牙本质侵蚀。
- 应控制NaOCl和EDTA的暴露时间以减少对牙本质基质的过度降解。
以上解读依据论文摘要(全文未开放获取或许可不允许翻译转载)。
原文
AIM: To characterize chemical degradation of the principal constituents of dentine after exposure to NaOCl and EDTA using Infrared Spectroscopy (ATR-FTIR). METHODOLOGY: Ground dentine particles, from extracted permanent human molars, were passed through sieves of 38 to 1 000 μm to provide six size ranges. Portions (250 mg) of each size range were reacted with 5 mL of 2.5% NaOCl for 2-10 min; or 17% EDTA for 5-1440 min. Powders larger than 75 μm were also sequentially exposed to NaOCl/EDTA/NaOCl each for 10 min. All experiments were repeated five times. Reacted and unreacted powders were washed and dried. Particles larger than 75 μm were then reground. FTIR spectra of unground and reground reacted particles enabled assessment of particle surface versus bulk chemistry, respectively, plus estimation of reaction depth. Changes in the ratio of the 1 640 cm-1 collagen: 1 010 cm-1 phosphate peak height or its inverse were obtained. These were used to estimate surface and bulk fraction reacted and thus depth to which collagen or phosphate was reduced following immersion in NaOCl or EDTA, respectively. The data were analysed descriptively. RESULTS: Surface collagen fraction declined by ~40% within 2 min of NaOCl exposure, and plateaued at ~60% between 6-10 min. Bulk spectra showed average depth of collagen loss at 10 min was 16 ± 13 μm. Ten minute EDTA exposure caused ~60% loss of surface phosphate. Average depth of phosphate loss was 19 ± 12 μm and 89 ± 43 μm after 10 and 1 440 min EDTA immersion, respectively. Sequential NaOCl/EDTA immersion yielded a 62 ± 28 μm thick phosphate-depleted surface. Sequential NaOCl/EDTA/NaOCl treatment resulted in approximately 85 μm of collagen loss. CONCLUSIONS: Data revealed the sequential depletion of collagen by NaOCl and apatite by EDTA in dentine, simultaneously exposing the other moieties. Alternate exposure to NaOCl and EDTA therefore enhances the depth of erosion.
引用
- Ramírez-Bommer C, Gulabivala K, Ng YL, et al. Estimated depth of apatite and collagen degradation in human dentine by sequential exposure to sodium hypochlorite and EDTA: a quantitative FTIR study. Int Endod J. 2017. PMID: 28992357. doi:10.1111/iej.12864
供执业医师工作参考,不替代临床判断;数值与分级以指南原文为准。