文献速递牙体牙髓病口腔修复与种植

银纳米线改性玻璃离子水门汀的抗生物膜与力学性能

Antibiofilm and mechanical properties of silver nanowire-modified glass ionomer cement.
PubMed 文献 · J Dent · 2023-05-30

本研究将不同纳米银配方(0.05%wt和0.5%wt AgNW、0.05%wt和0.5%wt AgNP)加入玻璃离子水门汀(GIC),用变形链球菌生物膜培养72小时并结合SEM与荧光显微镜评估抗生物膜效果,按ISO 9917-1:2007测抗压强度并用VITA Easyshade比较颜色。结果显示所有纳米银改性组变形链球菌数量显著低于传统GIC(p<0.0001),各组抗压强度无显著差异,AgNW改性GIC的颜色变化显著小于AgNP改性GIC。结论为AgNW改性GIC具有更优抗生物膜效果、抗压强度与传统GIC相当,且对颜色稳定性的影响小于AgNP。

要点

  • 所有纳米银改性GIC的变形链球菌数量均显著低于传统GIC(p<0.0001)。
  • 各组抗压强度无显著差异,0.5% AgNP组数值略低但无统计学意义。
  • AgNW改性GIC的颜色变化显著小于AgNP改性GIC,颜色稳定性更好。

核心结论

  • AgNW改性GIC抗生物膜效果优于传统GIC,抗压强度与之相当。
  • AgNW对GIC颜色稳定性的影响小于AgNP。

研究设计与样本

  • 体外研究:将0.05%wt和0.5%wt AgNW及0.05%wt和0.5%wt AgNP加入GIC。
  • 在GIC试件上培养变形链球菌生物膜72小时,用SEM观察并做SYTO-9荧光染色定量。
  • 按ISO 9917-1:2007测抗压强度,用VITA Easyshade系统比较颜色。

主要发现

  • SEM显示纳米银改性GIC表面积累的生物膜更少。
  • 所有纳米银改性组的变形链球菌数量均显著低于传统GIC(p<0.0001)。
  • 0.5% AgNP改性GIC抗压强度为58.3 ± 12.9 MPa,阴性对照为78.3 ± 13.8 MPa,但各组间无显著差异。
  • AgNW改性GIC与传统GIC之间的颜色变化显著低于AgNP改性GIC与传统GIC之间的颜色变化。

关键数值与推荐

  • 抗压强度评估依据ISO 9917-1:2007。
  • 变形链球菌生物膜培养时间为72小时。
  • 纳米银配方包括0.05%wt AgNW、0.5%wt AgNW、0.05%wt AgNP和0.5%wt AgNP。

临床怎么用

  • AgNW改性GIC在保持抗压强度的同时增强抗生物膜性能,具有临床转化潜力。
  • AgNW对颜色稳定性影响较小,适合对美观有要求的修复场景。

局限性

  • 原文未报告样本量、置信区间及除p<0.0001外的具体P值。
  • 仅使用变形链球菌单一菌种生物膜进行体外评估。
  • 颜色比较仅使用VITA Easyshade系统,未报告长期颜色稳定性数据。

以上解读依据论文摘要(全文未开放获取或许可不允许翻译转载)。

原文

BACKGROUND: Glass ionomer cement (GIC) is a commonly used restorative material in dentistry, but GIC does not have significant antibiofilm effects and its mechanical strength is limited. OBJECTIVE: To investigate the antibiofilm and mechanical properties of a newly developed silver nanowire (AgNW) modified GIC. METHODS: GICs were modified with different nanosilver formulations including 0.05%wt AgNW, 0.5%wt AgNW, 0.05%wt silver nanoparticle (AgNP) and 0.5%wt AgNP. Biofilms of Streptococcus mutans were cultured for 72 h on GIC specimens. Scanning electron microscopy (SEM) was conducted to observe the accumulation and morphology of Streptococcus mutans on the material surfaces. Another set of biofilm/specimens was treated with SYTO-9 and the biofilm development was evaluated by quantifying the visible stain with an inverted fluorescence microscope. The compressive strength of the specimens was assessed according to ISO 9917-1:2007. The colour of GICs was compared using the VITA Easyshade system. RESULTS: SEM images showed that fewer biofilms were accumulated on nanosilver-modified GICs. The Streptococcus mutans quantity was significantly lower in all nanosilver-modified groups compared to conventional GIC (p<0.0001). GIC modified with 0.5% AgNP showed slightly lower compressive strength than the negative control (58.3 ± 12.9 MPa vs 78.3 ± 13.8 MPa); but there is no significant difference between all study groups. The colour change between AgNW-modified GIC and conventional GIC was significantly lower than that between AgNP-modified GIC and conventional GIC. CONCLUSION: AgNW-modified GIC showed superior antibiofilm effect and comparable compressive strength to conventional GIC. In addition, the complement of AgNW would not influence the colour stability of GIC as much as AgNP. CLINICAL SIGNIFICANCE: This study developed a novel AgNW-modified GIC material. It showed good antibiofilm and mechanical properties and would not influence the colour stability of GIC. The AgNW-modified GIC has a large potential for clinical use and biomedical application.

来源:J Dent,查看原文。版权归原作者所有。

引用

  1. Guo T, Yang M, Wang D, et al. Antibiofilm and mechanical properties of silver nanowire-modified glass ionomer cement. J Dent. 2023. PMID: 37263409. doi:10.1016/j.jdent.2023.104569

供执业医师工作参考,不替代临床判断;数值与分级以指南原文为准。